Skip to main content

Stress-Strain Curve

What is a stress-strain curve?​

A stress-strain curve (also called a stress-strain graph or diagram) plots the stress in a material against its strain as it is stretched, usually in a tensile test until it breaks. Stress is force per unit area; strain is the stretch per unit of original length. Its shape gives a material's stiffness, yield strength, ultimate tensile strength and ductility.

A simulated tensile test of mild steel: engineering stress in MPa against strain in per cent, rising steeply, levelling off at the yield point, climbing through strain hardening to the ultimate tensile strength at 381 MPa and falling to fracture at 25% strain, with a second chart zoomed in on the first 1% of strain showing the dashed 0.2% offset line meeting the curve at the yield strength, in a dark navy theme

A simulated tensile test on mild steel, with the start of the curve enlarged on the right to show the 0.2% offset construction (sample data). Try the interactive version.

Key takeaways
  • Strain goes on the x-axis and stress on the y-axis. The curve is measured in a tensile test to standards such as ASTM E8/E8M or ISO 6892-1.
  • The first straight part is elastic: its slope is Young's modulus, and the material springs back when unloaded.
  • Most metals have no sharp yield point, so yield strength is read with the 0.2% offset method.
  • The peak is the ultimate tensile strength (UTS). After it the specimen necks, and the engineering stress falls until fracture.
  • Ductile materials stretch a long way before breaking; brittle ones, such as grey cast iron, break with almost no plastic strain.

How a tensile test produces the curve​

In a tensile test, a specimen of standard shape is gripped at both ends in a test machine and pulled apart at a controlled rate until it breaks. Metals are tested to ASTM E8/E8M or ISO 6892-1, plastics to ISO 527 or ASTM D638. The machine records two things many times a second:

  • the force, from a load cell;
  • the extension of a marked length in the middle of the specimen, the gauge length L0L_0, from an extensometer clipped to it.

Neither raw reading can be compared between specimens of different sizes, so both are normalised by the specimen's original dimensions:

σ=FA0ε=ΔLL0\sigma = \frac{F}{A_0} \qquad \varepsilon = \frac{\Delta L}{L_0}

where σ\sigma is the engineering stress (in MPa, which is N/mm²), FF the force, A0A_0 the original cross-sectional area, ε\varepsilon the engineering strain and ΔL\Delta L the extension. Strain has no units; it is usually shown in per cent.

As an example, take a round aluminium alloy bar 12.5 mm in diameter with a 62.5 mm gauge length (five diameters, the proportional specimen in ASTM E8M and ISO 6892-1). Its area is π×6.252≈122.7\pi \times 6.25^2 \approx 122.7 mm². A force of 20 kN gives a stress of 20,000/122.7≈16320{,}000 / 122.7 \approx 163 MPa, and an extension of 0.148 mm gives a strain of 0.148/62.5=0.002370.148 / 62.5 = 0.00237, or 0.237%. Plotting every pair of readings this way traces the stress-strain curve.

How to read a stress-strain curve​

A stress-strain curve is read from the origin outwards: a straight elastic region, the yield point, strain hardening up to the ultimate tensile strength, then necking and fracture.

An annotated stress-strain curve of a ductile metal, not to scale: a straight elastic region whose slope is Young's modulus up to the proportional limit, a dashed line parallel to it starting at 0.2% strain that meets the curve at the yield strength, a strain hardening region rising to the ultimate tensile strength, and a necking region falling to fracture, with the uniform elongation and the elongation at fracture marked on the strain axis

Read the curve from the origin outwards, one region at a time.

Elastic region and Young's modulus​

At first, stress rises in proportion to strain. This is Hooke's law:

σ=E ε\sigma = E\,\varepsilon

The constant EE is Young's modulus (the modulus of elasticity), the slope of this straight part. It measures stiffness: a steel at about 200 GPa stretches a third as much as an aluminium alloy at about 70 GPa under the same stress. In the elastic region, the atoms are pulled slightly apart but not rearranged, so the specimen returns to its original length when the load is removed.

To find Young's modulus from a stress-strain curve, take the slope of the straight part: E=Δσ/ΔεE = \Delta\sigma / \Delta\varepsilon. For the aluminium bar above, 10 kN gives 81.5 MPa at 0.118% strain and 20 kN gives 163.0 MPa at 0.236%, so

E=163.0−81.50.00236−0.00118≈69,000 MPa=69 GPaE = \frac{163.0 - 81.5}{0.00236 - 0.00118} \approx 69{,}000 \text{ MPa} = 69 \text{ GPa}

Test software fits a least-squares line through many readings in this range rather than using two points. ASTM E111 covers measuring the modulus itself, which needs a more precise extensometer than an ordinary tensile test.

Proportional limit and elastic limit​

The proportional limit is the highest stress at which the curve is still a straight line. The elastic limit is the highest stress the material can take and still return fully to its original length. For most metals the two are close together and hard to pin down, because the curve bends away from the line gradually. Neither is used as a design figure; the yield strength is.

Yield strength and the 0.2% offset method​

Yield strength is the stress at which the material starts to deform permanently (plastically). Some low-carbon steels show a clear yield point: the stress peaks (the upper yield point), drops slightly (the lower yield point) and runs flat for a while as bands of yielded metal, called Lüders bands, spread along the specimen. Most other metals, such as aluminium alloys, copper and stainless steel, bend smoothly from elastic to plastic with no sharp point.

For those, the 0.2% offset method gives a repeatable value:

  1. Draw a line with slope EE, parallel to the elastic part, starting at a strain of 0.2% (0.002) instead of at the origin.
  2. Find where this line crosses the curve.
  3. The stress there is the 0.2% offset yield strength, written Rp0.2R_{p0.2} in ISO 6892-1 and called the proof strength (often proof stress).

It means the stress that leaves 0.2% of permanent strain after the load is taken off. For the aluminium bar, the offset line is σ=69,000 (ε−0.002)\sigma = 69{,}000\,(\varepsilon - 0.002). At a force of 33.9 kN the curve reads 276 MPa at 0.600% strain, and the line gives 69,000×(0.006−0.002)=27669{,}000 \times (0.006 - 0.002) = 276 MPa: they cross, so the yield strength is 276 MPa. At 30 kN (244.5 MPa, 0.359%) the curve is still above the line; by 36 kN it has passed below it.

For plastics, ISO 527 defines the yield point differently: it is the first point where the strain increases without the stress increasing, the top of the first peak.

Strain hardening and ultimate tensile strength​

After yielding, the stress keeps rising, but more slowly. This is strain hardening (work hardening): the plastic deformation multiplies and tangles the dislocations in the metal's crystals, so each further increment of strain takes more stress. The specimen stretches evenly along its whole gauge length in this region.

The highest point on the curve is the ultimate tensile strength (UTS), also called the tensile strength RmR_m: the maximum force divided by the original area. For the aluminium bar, a maximum force of 38.0 kN gives a UTS of 310 MPa. The strain at that point is the uniform elongation.

Necking and fracture​

At the UTS, the deformation stops being even. One short section starts to thin faster than the rest and forms a neck. The neck's cross-section shrinks faster than the metal hardens, so the force needed to keep stretching it falls, and the engineering stress, still divided by the original area, falls with it. The specimen breaks in the neck.

The elongation after fracture is the permanent increase in gauge length after the break, in per cent of L0L_0. It is the usual measure of ductility, together with the reduction of area, the change in cross-section at the break.

Ductile vs brittle stress-strain curves​

The shape of the curve sorts materials into ductile and brittle ones. A ductile material yields and stretches well beyond its elastic limit before breaking; a brittle one breaks at or soon after the end of its elastic region, with little warning.

MaterialYoung's modulus (GPa)Yield strength (MPa)Tensile strength (MPa)Elongation (%)Shape of the curve
Low-carbon steel, 1020 hot rolled20721038025Ductile: sharp yield point and plateau, long strain hardening, necking
Aluminium alloy 6061-T66927631012Ductile: smooth bend into yield, short strain hardening, necking
Grey cast iron, grade G300066 to 97Not defined207 (minimum)Below 1Brittle: curved from the start, breaks at the top of the curve
Polycarbonate2.386263 to 72110 to 150Ductile polymer: yield peak, drop as a neck forms, long flat cold drawing, then a rise to break

Typical room-temperature values, from Callister and Rethwisch's tables. Real values depend on the grade, heat treatment, specimen and test speed, so use the supplier's certified figures for design.

What the table shows:

  • Stiffness and strength are different properties. Polycarbonate is about 90 times less stiff than the steel (2.38 against 207 GPa), but its yield strength is only about 3.4 times lower (62 against 210 MPa).
  • Grey cast iron has no yield strength: the graphite flakes in it act as small cracks, so it breaks before any useful plastic flow. Its curve is not even straight at the start, so its modulus depends on where the slope is taken.
  • Polycarbonate necks right at its yield peak, then the neck spreads along the whole specimen at an almost constant stress (cold drawing) as the polymer chains line up, so it can stretch to more than twice its length.
  • Temperature and loading rate change the shape. Steels can turn brittle in cold conditions, and plastics become stiffer and more brittle when pulled faster.

Engineering vs true stress-strain curves​

Engineering stress and strain use the specimen's original area and length. As the specimen stretches, its cross-section shrinks, so the real stress in the material is higher than the engineering stress. True stress divides the force by the actual area AA, and true strain adds up each small extension relative to the current length:

σT=FAεT=∫L0LdLL=ln⁡LL0\sigma_T = \frac{F}{A} \qquad \varepsilon_T = \int_{L_0}^{L}\frac{dL}{L} = \ln\frac{L}{L_0}

Metals keep their volume when they deform plastically (AL=A0L0A L = A_0 L_0), so while the specimen stretches evenly, both can be worked out from the engineering values:

σT=σ (1+ε)εT=ln⁡(1+ε)\sigma_T = \sigma\,(1 + \varepsilon) \qquad \varepsilon_T = \ln(1 + \varepsilon)

At the aluminium bar's UTS (310 MPa at 8% engineering strain), the true stress is 310×1.08≈335310 \times 1.08 \approx 335 MPa and the true strain is ln⁡1.08≈0.077\ln 1.08 \approx 0.077. At small strains the two curves are almost the same; they draw apart as the strain grows.

These two formulas only hold up to the start of necking. After that, the strain is concentrated in the neck, and the true stress has to be found by measuring the neck's diameter. Drawn that way, the true stress keeps rising until fracture, because the metal in the neck is still hardening.

Necking starts when the hardening can no longer make up for the shrinking area. In true terms, that is when the slope of the true curve falls to the true stress itself, dσT/dεT=σTd\sigma_T / d\varepsilon_T = \sigma_T (Considère's criterion). Use the engineering curve for design limits and material specifications, and the true curve for modelling plastic forming and crash behaviour, where finite element programs expect true stress against true plastic strain.

Engineering curveTrue curve
StressForce over original area, F/A0F/A_0Force over actual area, F/AF/A
StrainΔL/L0\Delta L / L_0ln⁡(L/L0)\ln(L/L_0)
After the UTSFalls until fractureKeeps rising until fracture
Used forSpecifications, data sheets, design allowablesMetal forming, plasticity models, simulation input

Toughness and resilience: the area under the curve​

The area under a stress-strain curve is the energy absorbed per unit volume of material. Stress in MPa times strain gives MJ/m³.

  • The modulus of resilience is the area under the elastic part, up to yield: the energy a material can store and give back without permanent damage. For a straight elastic line it is a triangle, Ur=σy2/2EU_r = \sigma_y^2 / 2E. For the aluminium alloy, 2762/(2×69,000)≈0.55276^2 / (2 \times 69{,}000) \approx 0.55 MJ/m³; for the 1020 steel, 2102/(2×207,000)≈0.11210^2 / (2 \times 207{,}000) \approx 0.11 MJ/m³. Springs are made from materials with a high yield strength and a modest modulus for this reason.
  • Toughness (tensile toughness) is the area under the whole curve to fracture: the energy needed to break the material. A rough estimate for a ductile metal is the average of yield strength and UTS times the strain at fracture, (210+380)/2×0.25≈74(210 + 380)/2 \times 0.25 \approx 74 MJ/m³ for the steel. Grey cast iron, with a similar tensile strength but under 1% strain, absorbs less than a hundredth of that.

Tensile toughness is not the same as fracture toughness, which measures resistance to a crack that is already there and comes from a different test.

S-N curves: stress-strain's fatigue counterpart​

A stress-strain curve describes one pull to failure. Parts that are loaded and unloaded millions of times, such as shafts, springs, aircraft skins and bridges, can fail by fatigue at stresses well below the yield strength. The curve for that is the S-N curve (or Wöhler curve): the stress amplitude SS against the number of cycles to failure NN, from tests in which specimens are loaded back and forth at a fixed stress until they break (ASTM E466, ISO 1099).

S-N curves on logarithmic axes from a thousand to a billion cycles: a steel line falls from about 342 MPa at 1,000 cycles to a knee at about 190 MPa near one million cycles and then runs flat, the endurance limit; a dashed aluminium alloy line keeps falling with no knee, with its fatigue strength marked at 500 million cycles; scattered test points sit around the steel line

Both axes are almost always on a log scale, because the lives span several powers of ten. On log-log axes much of the curve is close to a straight line, Basquin's relation S=aNbS = a N^b, with bb typically around −0.05 to −0.12 for metals.

  • Steels and titanium alloys usually show a knee and then a flat line, the endurance limit. Below it, a smooth specimen is expected to survive indefinitely, in normal conditions without corrosion. A common first estimate for steels with a UTS up to about 1,400 MPa is an endurance limit of half the UTS, and a fatigue strength at 1,000 cycles of about 0.8 to 0.9 × UTS in bending, depending on strength. The steel line in the diagram uses 0.9.
  • Aluminium and copper alloys have no knee: the line keeps falling. Their fatigue strength is quoted at a stated life, often 10710^7 or 5×1085 \times 10^8 cycles.
  • Fatigue lives scatter widely, and can differ by a factor of ten or more at the same stress, so curves are fitted statistically (as in ISO 12107) and design curves sit well below the average. Surface finish, notches, size and mean stress all lower them further.

Common stress-strain curve mistakes​

Most stress-strain curve mistakes come from reading the yield in the wrong place or from measuring strain in the wrong way.

  • Reading the yield at the end of the straight line. The proportional limit is subjective and depends on the resolution of the plot. Use the 0.2% offset, or the lower yield point for steels with a plateau, so results can be compared.
  • Taking the modulus from the crosshead. Without an extensometer, the strain includes the stretch of the grips and the machine, and the slope comes out well below the real modulus. The yield and UTS are still usable; the modulus is not.
  • Using the wrong offset line. The offset line must have the modulus's slope and start at 0.2% strain. If the curve has a toe at the start, from the grips settling, shift the origin to where the straight part extended meets zero stress (toe compensation, described in ASTM D638 for plastics).
  • Mixing engineering and true values. Data sheets give engineering values; simulation programs usually want true stress against true plastic strain. Converting past the UTS with σ(1+ε)\sigma(1+\varepsilon) is wrong, because the strain is no longer even.
  • Comparing elongations from different gauge lengths. Most of the strain at fracture is in the neck, so a short gauge length gives a higher elongation than a long one for the same material. Quote the gauge length with the elongation, as ISO 6892-1 does with AA and A50mmA_{50\text{mm}}.
  • Ignoring strain rate and temperature. A polymer or a mild steel tested faster or colder shows a higher yield and less elongation. Compare curves only from the same test conditions.
  • Plotting strain on a squashed axis. Over the whole curve of a ductile metal, the elastic region takes up less than 1% of the strain axis and looks vertical. Show an enlarged view of the start of the curve when the modulus or yield matters.

How to plot a stress-strain curve in JavaScript, React or Angular​

Test machines sample force and extension hundreds of times a second, and a materials lab compares curves from many specimens and batches. The demo below simulates a tensile test on four materials with typical published properties, about 2,500 readings per test, then works out the modulus, yield strength, UTS and elongation from the data as test software does, and can replay the test point by point as a machine draws it.

Choose a Material, and switch the Curve between engineering stress, true stress (drawn up to the start of necking) and both. 0.2% offset construction draws the offset line and marks where it meets the curve; the right-hand chart enlarges the start of the curve, where the modulus and yield are read. Shade resilience and toughness fills the areas under the curve, and Run test replays the test as a machine would draw it, slowly through the elastic region and faster after it. Hover for stress and strain; the mouse wheel zooms, dragging pans and a double-click resets.

Here is the code for this chart. The test analysis (modulus fit, offset yield, true stress and areas) is plain JavaScript; SciChart.js draws the curves, the offset line, the shaded areas and the labelled points.

// Read Young's modulus, yield strength (0.2% offset), UTS and elongation from a tensile test, and chart it with SciChart.js
const {
SciChartSurface,
NumericAxis,
NumberRange,
EAutoRange,
FastLineRenderableSeries,
FastMountainRenderableSeries,
XyScatterRenderableSeries,
EllipsePointMarker,
XyDataSeries,
TextAnnotation,
EHorizontalAnchorPoint,
EVerticalAnchorPoint,
SciChartJsNavyTheme,
LegendModifier,
ELegendPlacement,
CursorModifier,
MouseWheelZoomModifier,
ZoomPanModifier,
ZoomExtentsModifier
} = SciChart;
// or, for npm, import { SciChartSurface, ... } from "scichart"

// --- Tensile test analysis (plain JavaScript, no library needed). Strain is a fraction, stress in MPa ---

// Young's modulus: the slope of a least-squares straight line through the points in the fitting range
function fitModulus(strain, stress, inFitRange) {
let n = 0, sx = 0, sy = 0, sxx = 0, sxy = 0;
for (let i = 0; i < strain.length; i++) {
if (!inFitRange(strain[i], stress[i]) || strain[i] > 0.05) continue;
n++;
sx += strain[i];
sy += stress[i];
sxx += strain[i] * strain[i];
sxy += strain[i] * stress[i];
}
const slope = (n * sxy - sx * sy) / (n * sxx - sx * sx);
return { E: slope, intercept: (sy - slope * sx) / n };
}

// 0.2% offset yield strength: where the curve meets a line of slope E shifted 0.002 along the strain axis
function offsetYield(strain, stress, fit, offset = 0.002) {
const shift = offset - fit.intercept / fit.E; // the elastic line starts where the fitted line crosses zero stress
const gap = (i) => stress[i] - fit.E * (strain[i] - shift);
for (let i = 1; i < strain.length; i++) {
if (strain[i] > shift && gap(i) <= 0 && gap(i - 1) > 0) {
const t = gap(i - 1) / (gap(i - 1) - gap(i));
return { strain: strain[i - 1] + t * (strain[i] - strain[i - 1]), stress: stress[i - 1] + t * (stress[i] - stress[i - 1]), shift };
}
}
return null; // broke before yielding
}

// Area under the curve (trapezium rule) up to a strain. MPa x strain = MJ/m³
function areaUnder(strain, stress, upTo) {
let area = 0;
for (let i = 1; i < strain.length && strain[i - 1] < upTo; i++) {
const e1 = Math.min(strain[i], upTo);
const s1 = stress[i - 1] + ((stress[i] - stress[i - 1]) * (e1 - strain[i - 1])) / (strain[i] - strain[i - 1] || 1);
area += ((stress[i - 1] + s1) / 2) * (e1 - strain[i - 1]);
}
return area;
}

// True stress and strain, valid while the specimen stretches evenly (up to the start of necking)
function toTrue(strain, stress, upTo) {
const e = [];
const s = [];
for (let i = 0; i < strain.length - 1 && strain[i] <= upTo; i++) { // the last point is the break
e.push(Math.log(1 + strain[i]));
s.push(stress[i] * (1 + strain[i]));
}
return { strain: e, stress: s };
}

// --- Two charts: the whole curve, and the start of the curve, where the modulus and yield are read ---
async function createChart(div, title) {
const { sciChartSurface, wasmContext } = await SciChartSurface.create(div, {
theme: new SciChartJsNavyTheme(),
title,
titleStyle: { fontSize: 15 }
});
const xAxis = new NumericAxis(wasmContext, { axisTitle: "Strain (%)", labelPrecision: 1 });
const yAxis = new NumericAxis(wasmContext, { axisTitle: "Stress (MPa)", autoRange: EAutoRange.Always, growBy: new NumberRange(0, 0.12), labelPrecision: 0 });
sciChartSurface.xAxes.add(xAxis);
sciChartSurface.yAxes.add(yAxis);
const add = (series) => series; // added to the chart in draw(), when shown
const data = (name) => new XyDataSeries(wasmContext, { dataSeriesName: name });
const series = {
toughness: add(new FastMountainRenderableSeries(wasmContext, { dataSeries: data("Toughness (area to fracture)"), fill: "#50C7E044", stroke: "#50C7E088", strokeThickness: 1 })),
resilience: add(new FastMountainRenderableSeries(wasmContext, { dataSeries: data("Resilience (elastic energy to yield)"), fill: "#F48420AA", stroke: "#F48420", strokeThickness: 1 })),
engineering: add(new FastLineRenderableSeries(wasmContext, { dataSeries: data("Engineering stress-strain"), stroke: "#50C7E0", strokeThickness: 2.5 })),
trueCurve: add(new FastLineRenderableSeries(wasmContext, { dataSeries: data("True stress-strain (to necking)"), stroke: "#F5E663", strokeThickness: 2.5 })),
offsetLine: add(new FastLineRenderableSeries(wasmContext, { dataSeries: data("0.2% offset line"), stroke: "#EC0F6C", strokeThickness: 2, strokeDashArray: [6, 4] })),
points: add(new XyScatterRenderableSeries(wasmContext, {
dataSeries: data("Yield, UTS and fracture"),
pointMarker: new EllipsePointMarker(wasmContext, { width: 11, height: 11, fill: "#FFFFFF", stroke: "#EC0F6C", strokeThickness: 2 })
}))
};
sciChartSurface.chartModifiers.add(
new CursorModifier({ showTooltip: true, showAxisLabels: false }),
new MouseWheelZoomModifier(),
new ZoomPanModifier(),
new ZoomExtentsModifier()
);
return { sciChartSurface, xAxis, yAxis, series, shown: "" };
}

// Show only the series that are switched on, so the legend lists just those. Re-adding in a fixed order keeps
// the shaded areas behind the lines.
function showSeries(chart, visible) {
const key = Object.keys(chart.series).filter((name) => visible[name]).join();
if (key === chart.shown) return;
chart.shown = key;
chart.sciChartSurface.renderableSeries.clear(false);
for (const name of Object.keys(chart.series)) if (visible[name]) chart.sciChartSurface.renderableSeries.add(chart.series[name]);
}
const main = await createChart(ui.mainDiv, "Tensile test");
const zoom = await createChart(ui.zoomDiv, "Start of the curve");
zoom.yAxis.autoRange = EAutoRange.Never; // its range is set in draw(), from the part of the curve it shows
main.sciChartSurface.chartModifiers.add(
new LegendModifier({ placement: ELegendPlacement.BottomRight, showCheckboxes: false, backgroundColor: "#14233CCC" })
);

const setData = (series, xs, ys) => {
series.dataSeries.clear();
series.dataSeries.appendRange(xs.map((v) => v * 100), ys); // strain as a percentage
};

let test; // the current material's results
let animation = 0; // id of the running "test", so a new one cancels the old

function analyse() {
const m = MATERIALS[ui.materialSelect.value];
const { strain, stress, neckingStrain } = simulateTensileTest(m);
const peak = stress.reduce((best, s, i) => (s > stress[best] ? i : best), 0);
// Metals: fit between 10% and 40% of the yield strength (UTS for cast iron). Plastics (ISO 527): 0.05% to 0.25% strain
const reference = m.yieldStrength || m.uts;
const fit = m.shape === "polymer"
? fitModulus(strain, stress, (e) => e >= 0.0005 && e <= 0.0025)
: fitModulus(strain, stress, (e, s) => s >= 0.1 * reference && s <= 0.4 * reference);
let yieldPoint = null;
let yieldMethod = "";
if (m.shape === "polymer") {
// Plastics (ISO 527): the yield point is the first maximum, where the stress stops rising
// (the highest point before the stress has fallen 5% below it)
let best = strain.findIndex((e) => e > 0.01);
for (let i = best; i < stress.length && stress[i] > 0.95 * stress[best]; i++) if (stress[i] > stress[best]) best = i;
yieldPoint = { strain: strain[best], stress: stress[best] };
yieldMethod = "first maximum";
} else if (m.shape !== "brittle") {
yieldPoint = offsetYield(strain, stress, fit);
yieldMethod = "0.2% offset";
}
const fractureIndex = stress.length - 2; // the last point before the load falls to zero
test = {
m, strain, stress, fit, yieldPoint, yieldMethod, neckingStrain,
uts: { strain: strain[peak], stress: stress[peak] },
fracture: { strain: strain[fractureIndex], stress: stress[fractureIndex] },
elongation: strain[fractureIndex] - stress[fractureIndex] / fit.E, // permanent strain after the break
// Modulus of resilience: the elastic energy stored up to yield, the triangle under the straight line, yield² / 2E
resilience: yieldPoint ? (yieldPoint.stress * yieldPoint.stress) / (2 * fit.E) : NaN,
toughness: areaUnder(strain, stress, strain[fractureIndex])
};
}

function draw(upToStrain) {
const { m, strain, stress, fit, yieldPoint, uts, fracture } = test;
const finished = upToStrain >= m.fractureStrain;
const curve = ui.curveSelect.value;
const visibleCount = finished ? strain.length : strain.findIndex((e) => e > upToStrain);
const xs = strain.slice(0, visibleCount);
const ys = stress.slice(0, visibleCount);
const trueCurve = toTrue(strain, stress, Math.min(test.neckingStrain, upToStrain));

for (const chart of [main, zoom]) {
const s = chart.series;
setData(s.engineering, xs, ys);
setData(s.trueCurve, trueCurve.strain, trueCurve.stress);
const showOffset = finished && ui.offsetCheckbox.checked && test.yieldMethod === "0.2% offset";
if (showOffset) {
const end = yieldPoint.strain + 0.4 * (yieldPoint.strain - yieldPoint.shift);
setData(s.offsetLine, [yieldPoint.shift, end], [0, fit.E * (end - yieldPoint.shift)]);
}
const areas = finished && ui.areasCheckbox.checked && curve !== "true";
if (areas) {
setData(s.toughness, strain.slice(0, -1), stress.slice(0, -1));
if (yieldPoint) setData(s.resilience, [0, yieldPoint.stress / fit.E], [0, yieldPoint.stress]);
}
const keyPoints = finished ? [yieldPoint, uts, fracture].filter(Boolean) : [];
showSeries(chart, {
toughness: areas,
resilience: areas && !!yieldPoint,
engineering: curve !== "true",
trueCurve: curve !== "engineering",
offsetLine: showOffset,
points: finished && curve !== "true"
});
setData(s.points, keyPoints.map((p) => p.strain), keyPoints.map((p) => p.stress));

chart.sciChartSurface.annotations.clear();
if (finished && curve !== "true") {
// Labels on the right of a point, or on its left near the end of the strain axis
const label = (p, text, below) => {
const left = p.strain > 0.75 * m.fractureStrain && chart === main;
return new TextAnnotation({
x1: p.strain * 100,
y1: p.stress,
text,
fontSize: 13,
textColor: "#FFFFFF",
horizontalAnchorPoint: left ? EHorizontalAnchorPoint.Right : EHorizontalAnchorPoint.Left,
verticalAnchorPoint: below ? EVerticalAnchorPoint.Top : EVerticalAnchorPoint.Bottom,
xCoordShift: left ? -8 : 8,
yCoordShift: below ? 8 : -6
});
};
if (yieldPoint) chart.sciChartSurface.annotations.add(label(yieldPoint, `Yield ${yieldPoint.stress.toFixed(0)} MPa`, m.shape !== "polymer"));
if (chart === main) {
chart.sciChartSurface.annotations.add(label(uts, `UTS ${uts.stress.toFixed(0)} MPa`, false));
chart.sciChartSurface.annotations.add(label(fracture, "Fracture", true));
}
}
}
// Fixed x-ranges, so the curve grows across the chart during a test
main.xAxis.visibleRange = new NumberRange(0, m.fractureStrain * 100 * 1.05);
main.xAxis.labelProvider.precision = m.fractureStrain < 0.05 ? 2 : 0;
zoom.xAxis.visibleRange = new NumberRange(0, m.zoomStrain);
let zoomTop = 0;
for (let i = 0; i < strain.length && strain[i] * 100 <= m.zoomStrain; i++) zoomTop = Math.max(zoomTop, stress[i] * (curve === "engineering" ? 1 : 1 + strain[i]));
zoom.yAxis.visibleRange = new NumberRange(0, zoomTop * 1.2);

const fmt = (v, digits) => (Number.isFinite(v) ? v.toFixed(digits) : "–");
if (!finished) {
const last = visibleCount - 1;
ui.readout.textContent = `Testing… strain ${fmt(strain[last] * 100, 2)}%, stress ${fmt(stress[last], 0)} MPa`;
return;
}
ui.readout.textContent =
`E ${fmt(fit.E / 1000, fit.E < 10000 ? 1 : 0)} GPa · ` +
(yieldPoint ? `Yield (${test.yieldMethod}) ${fmt(yieldPoint.stress, 0)} MPa · ` : "No yield: breaks first · ") +
`UTS ${fmt(uts.stress, 0)} MPa · Elongation after fracture ${fmt(test.elongation * 100, 1)}% · ` +
(yieldPoint ? `Resilience ${fmt(test.resilience, 2)} MJ/m³ · ` : "") +
`Toughness ${fmt(test.toughness, test.toughness < 10 ? 2 : 0)} MJ/m³`;
}

// "Run test": draw the curve as a test machine would, slowly through the elastic region and faster after it
function runTest() {
const id = ++animation;
const started = performance.now();
const duration = 6000; // ms
const step = () => {
if (id !== animation || main.sciChartSurface.isDeleted) return;
const t = Math.min(1, (performance.now() - started) / duration);
draw(t >= 1 ? Infinity : test.m.fractureStrain * t * t);
if (t < 1) requestAnimationFrame(step);
};
step();
}

function onMaterialChanged() {
animation++; // stop any test in progress
analyse();
draw(Infinity);
}
ui.materialSelect.addEventListener("change", onMaterialChanged);
for (const control of [ui.curveSelect, ui.offsetCheckbox, ui.areasCheckbox]) {
control.addEventListener("change", () => {
animation++;
draw(Infinity);
});
}
ui.runButton.addEventListener("click", runTest);
onMaterialChanged();

Key points:

  • Each curve is a FastLineRenderableSeries over an XyDataSeries, with strain in per cent on the x-axis. The 0.2% offset line is a second line series with strokeDashArray, and the yield, UTS and fracture points are an XyScatterRenderableSeries with an EllipsePointMarker, labelled with TextAnnotations.
  • The resilience and toughness areas are FastMountainRenderableSeries, which fill down to zero stress. The controls add and remove series from renderableSeries in a fixed order, so the legend lists only what is shown and the areas stay behind the lines.
  • Two SciChartSurfaces show the same test: the whole curve, and the start of the curve on a fixed range, so the modulus and offset construction stay readable next to a strain axis that runs to 25% or 110%.
  • Run test appends points frame by frame with requestAnimationFrame, which is how you would stream readings from a live test machine; the chart redraws on each update.

See it in the demo app: JavaScript line chart · React line chart · Angular line chart, and for labelled points and lines, JavaScript chart annotations · React chart annotations · Angular chart annotations.

Go deeper: SciChart.js line series documentation, the mountain (area) series documentation and the scatter series documentation. For how test and measurement teams use SciChart in their software, see SciChart for design, emulation and test and SciChart for instrumentation engineering. To inspect parts without breaking them, see non-destructive testing.

Frequently asked questions​

What does a stress-strain curve tell you?​

A stress-strain curve tells you how a material responds as it is stretched until it breaks. From it you read the stiffness (Young's modulus, the slope of the first straight part), the stress at which permanent deformation starts (yield strength), the highest stress it can carry (ultimate tensile strength), how far it stretches before breaking (elongation, a measure of ductility) and the energy it absorbs (toughness, the area under the curve).

How do you find Young's modulus from a stress-strain curve?​

Young's modulus is the slope of the straight, elastic part at the start of the curve: the change in stress divided by the change in strain between two points on it. Fit a straight line through the readings in that region rather than using two single points, because the first few readings are often affected by the grips settling. Steels come out at about 200 GPa and aluminium alloys at about 70 GPa.

How do you find the yield strength with the 0.2% offset method?​

Draw a straight line with the same slope as the elastic part of the curve (Young's modulus), starting at 0.2% strain (0.002) on the strain axis instead of at the origin. The stress where this line crosses the curve is the 0.2% offset yield strength, also called the 0.2% proof strength (often proof stress) or Rp0.2. It is the stress that leaves a permanent strain of 0.2% when the load is removed.

What is the difference between engineering and true stress-strain curves?​

Engineering stress divides the force by the specimen's original cross-section, and engineering strain divides the extension by the original length. True stress uses the actual, shrinking cross-section, and true strain adds up each small extension relative to the current length. Up to the start of necking, true stress = engineering stress × (1 + engineering strain) and true strain = ln(1 + engineering strain). The true curve keeps rising after the ultimate tensile strength, while the engineering curve falls.

Why does the stress drop after the ultimate tensile strength?​

After the ultimate tensile strength, the deformation concentrates in one short section of the specimen, which thins into a neck. The neck's cross-section shrinks faster than the metal there hardens, so the force needed to keep stretching it falls. Engineering stress is that force divided by the original area, so it falls too, even though the true stress in the neck is still rising.

How do I plot a stress-strain curve in JavaScript?​

Convert the test machine's force and extension readings to stress (force over original area, in MPa) and strain (extension over gauge length, often in %), and draw them as a line series with strain on the x-axis. Fit the modulus over the elastic region, find the 0.2% offset yield and the maximum stress in plain JavaScript, and mark them with a scatter series and text annotations. SciChart.js does this with FastLineRenderableSeries, XyScatterRenderableSeries and TextAnnotation, in plain JavaScript, React or Angular.

Sources​

  • ASTM E8/E8M, Standard Test Methods for Tension Testing of Metallic Materials, and ISO 6892-1, Metallic materials: Tensile testing, Part 1: Method of test at room temperature. Specimens, gauge lengths, the offset method, yield point, tensile strength and elongation after fracture.
  • ASTM E111, Standard Test Method for Young's Modulus, Tangent Modulus, and Chord Modulus; ISO 527-1, Plastics: Determination of tensile properties, for the yield point and modulus of plastics.
  • Callister, W. D. and Rethwisch, D. G. (2018), Materials Science and Engineering: An Introduction, 10th edition, Wiley. Chapter 6 (mechanical properties of metals) and the property tables in Appendix B, the source of the typical values above.
  • Roylance, D., Mechanics of Materials, MIT, on LibreTexts: Stress-strain curves. Engineering and true stress, Considère's construction and strain energy.
  • Budynas, R. G. and Nisbett, J. K. (2020), Shigley's Mechanical Engineering Design, 11th edition, McGraw-Hill. Chapter 6: S-N curves, the endurance limit estimate and the fatigue strength fraction at 1,000 cycles. ASTM E466 covers axial fatigue testing.
  • ISO 12107:2012, Metallic materials: Fatigue testing, Statistical planning and analysis of data. Fitting S-N curves to scattered fatigue lives.